תקציר
Ceramic BiFeO3 samples were prepared by rapid sintering at 880◦C. Two compositions were examined. A 56/44 Bi2O3/Fe2O3 mole% composition and a 56Bi2O3 44Fe2O3 + 6.5wt% NaCl composition. The samples were heat treated at different times up to 8 minutes and the phase content was examined as a function of the time using XRD measurements and analysis. It was demonstrated that using both compositions, maximum BiFeO3 phase content is obtained after 3.5 minutes. In the former approximately 50% of the material transformed to BiFeO3 while in the latter 98.5%.
שפה מקורית | אנגלית |
---|---|
עמודים (מ-עד) | 40-45 |
מספר עמודים | 6 |
כתב עת | Bulgarian Chemical Communications |
כרך | 52 |
מזהי עצם דיגיטלי (DOIs) | |
סטטוס פרסום | פורסם - 2020 |